Change Iconel Type and PWHT

10/01/2010 5:30 AM

We need weld P91 with ss-316L (Pipe to a thermo coupilng). My concerns are about to points:

1. Approved WPS require ERNICR3 (SFA N 5.14), But we have ERNICRMO 3 (Same SFA N 5.14) May I use this filler metal without WPS recualification?

2. Is possible to PWHT at 745ºC the SS- 316L? (For P91 is OK)

Thanks

Register to Reply
Interested in this topic? By joining CR4 you can "subscribe" to
this discussion and receive notification when new comments are added.
Commentator
Engineering Fields - Piping Design Engineering - New Member

Join Date: Apr 2010
Posts: 66
Good Answers: 1
#1

Re: Change Iconel Type and PWHT

10/08/2010 3:31 PM

In my opinion, buttering (if possible) of P91 side should be done followed by PWHT. After this, you weld the part to SS316L piping.

You must use ERNiCr-3 although F-numbers of both the wires are same but A-number is different and both are essential variables for GTAW. Or otherwise, re-qualify the welding procedure with ERNiCrMo-3.

Regards,

Ashfaq